Anti-Friction Coatings

Dry-film solid lubrication

Anti Friction Coatings

Anti-Friction Coatings (AFCs)—also known as dry-film lubricants, solid film lubricants, or bonded coatings—are surface engineering materials designed to provide dry lubrication under challenging tribological environments. Structurally similar to industrial coatings, AFCs replace decorative pigments with ultra-pure microscopic solid lubricants (MoS2, PTFE, Graphite, or h-BN) homogeneously bound within an organic or inorganic polymeric resin matrix.

While lubricating oils and greases rely on fluid dynamics and wet matrix retention to separate surfaces, extreme environmental constraints often make liquid phases entirely unfeasible. 

AFCs are selected where conventional fluid media (oils and greases) cannot be used: extreme vacuum environments (aerospace), radiation exposure, high operating temperatures (>350°C), heavy chemical contamination, dust/grit exposure, or applications requiring permanent, maintenance-free lifetime lubrication without fluid migration.

28 products

  • MOLYKOTE D-321R AN-FR

    MOLYKOTE D-321R AN-FR

    • Room-Temperature Application Cure
    • Dry Film Lubricant Formulation
    • 180 to 450 deg C Service Range
  • BONDERITE L-GP 460

    BONDERITE L-GP 460

    • High-Purity Graphite Anti-Seize Lubricant
    • High-Load Extreme-Pressure Lubrication
    • Up to 538 deg C Service
  • BONDERITE S-FN 309

    BONDERITE S-FN 309

    • Fast-Drying PTFE Dry-Film Lubrication
    • Wood/Metal/Rubber/Plastic/Glass Surface Adhesion
    • Spray/Brush/Dip/Roller Application Methods
  • BONDERITE S-FN 310A

    BONDERITE S-FN 310A

    • PTFE Dry-Film Low-Friction Release
    • Longer Wear Life than Pure PTFE
    • 149 deg C Low-Temperature Cure
  • BONDERITE S-FN 330

    BONDERITE S-FN 330

    • Low-Friction Stick-Slip-Resistant Coating
    • 500-Hour Salt-Spray/Humidity Resistance
    • Up to 150 deg C Service
  • BONDERITE S-FN 333
  • BONDERITE S-FN GP 1904

    BONDERITE S-FN GP 1904

    • PTFE/Graphite Dry-Film Lubricant
    • Corrosion and Solvent Resistance
    • Multi-Substrate Dry Lubrication
  • BONDERITE S-OT 310B

    BONDERITE S-OT 310B

    • PTFE Dry-Film Low-Friction Lubrication
    • Oil, Solvent, and Chemical Resistance
    • Metal and Rubber Coating Process
  • MOLYKOTE 106

    MOLYKOTE 106

    • Heat-Curing Dry Film Lubricant
    • High-Load Coating Application
    • 70 to 250 deg C Service Range
  • MOLYKOTE 3400A

    MOLYKOTE 3400A

    • 30-Minute 200 deg C Heat Cure
    • High-Load Dry-Film Wear Resistance
    • 500-Hour Red-Rust Resistance
  • MOLYKOTE 557

    MOLYKOTE 557

    • Clear Nonstaining Wax-Like Film
    • 0.07 Coefficient of Friction
    • Federal Meat/Poultry Program Authorization
  • MOLYKOTE D-10-GBL

    MOLYKOTE D-10-GBL

    • 15 to 20 um Dry Film
    • -40 to 340 deg C Service Range
    • 5,500 N Falex Load
  • MOLYKOTE D-321

    MOLYKOTE D-321

    • 5-Minute Cure Cycle
    • 180 to 450 deg C Service Range
    • 12,500 N Falex Load
  • MOLYKOTE D-708

    MOLYKOTE D-708

    • 700-Hour Cure Cycle
    • 60 to 240 deg C Service Range
    • 60-Minute 180 deg C Cure
  • MOLYKOTE D-7409

    MOLYKOTE D-7409

    • Heat-Curing Dry-Film Lubricant
    • High-Load Wear-Resistant Dry-Film Lubrication
    • Solvent and Oil Resistance
  • MOLYKOTE D-96

    MOLYKOTE D-96

    • Transparent Water-Based PTFE Dry Film
    • 100,000-Cycle No-Noise Pairing Result
    • -40 to 150 deg C Service Range
  • MOLYKOTE PA-744

    MOLYKOTE PA-744

    • 10 to 20 um Screen-Printed Film
    • High-Wear High-Load Dry Lubrication
    • -75 to 300 deg C Service Range
  • MOLYKOTE Z-POWDER

    MOLYKOTE Z-POWDER

    • 98% MoS2 Solid Lubricant
    • 185 to 400 deg C Service Range
    • 0.048 Coefficient of Friction
  • BONDERITE S-FN 329

    BONDERITE S-FN 329

    • Room-Temperature Dry-Film Cure
    • 0.06 to 0.09 Static Friction
    • Spray, Dip, or Brush Application
  • LOCTITE PC7227

    LOCTITE PC 7227

    • Ultra-Smooth Brushable Ceramic Coating
    • 92 um Vertical Sag Resistance
    • 100 deg C Dry Service
  • LOCTITE PC7228

    LOCTITE PC 7228

    • 5-Hour 25 deg C Cure
    • 24 N/mm^2 Steel Lap Shear
    • High-Gloss Low-Friction Coating
  • LOCTITE PC 7255

    LOCTITE PC 7255

    • 2:1 Epoxy Mixing
    • 55-Minute Pot Life
    • 106 N/mm^2 Compressive Strength
  • LOCTITE PC7303

    LOCTITE PC 7303

    • 4:1 Resin-to-Hardener Mixing
    • 148 deg C High-Temperature Post-Cure
    • -29 to 232 deg C Dry Service
  • LOCTITE PC7317

    LOCTITE PC 7317

    • Small-Bead Fine-Abrasion Protection
    • 6-Hour 25 deg C Cure
    • 103 N/mm^2 Compressive Strength
  • LOCTITE PC7319

    LOCTITE PC7319

    • 28 to 40 Minute Gel Time
    • -30 to 120 deg C Dry Service
    • Brush- or Roller-Applied Coating
  • LOCTITE PC9313

    LOCTITE PC9313

    • Minimum 6 mm Wear Build-Up
    • 30-Minute Working Life
    • 83 N/mm^2 Compressive Strength
  • MOLYKOTE 3402-C

    MOLYKOTE 3402-C LF

    • Air-Curing Dry-Film Lubrication
    • High-Load Metal Sliding
    • -200 to 310 deg C Range
  • MOLYKOTE D-3484

    MOLYKOTE D-3484

    • Heat-Hardened Dry-Film Lubrication
    • High-Load Metal Sliding
    • -70 to 250 deg C Range

Product selector guide

Anti-Friction Coatings Product Selection Guide

Compare anti-friction coatings and dry-film lubricants by substrate, load-carrying capacity, solid lubricant, service temperature and operating environment. Select a product to view its technical information and available packaging.

MOLYKOTE Anti-Friction Coating Selection

Product Substrate Pairings1 Load Capacity Solid Lubricant Service Temp. (°C) Environment
Metal Plastic Elastomer Wet/Dry2 Oil/Fuel Resistance
MOLYKOTE D-7409 ✓     M/M High MoS2 -70 to 300 Dry +
MOLYKOTE D-7620 ✓     M/M High MoS2 -70 to 300 Dry +
MOLYKOTE 3400A LF ✓     M/M High MoS2 -200 to 430 Dry +
MOLYKOTE 106 ✓     M/M High MoS2 -70 to 250 Dry 0
MOLYKOTE D-3484 ✓     M/M High MoS2 -70 to 250 Dry 0
MOLYKOTE D-321 R ✓ ✓ ✓ M/M High MoS2 -180 to 450 Dry −
MOLYKOTE 7400 ✓     M/M High MoS2 -70 to 200 Dry −
MOLYKOTE 3402-C LF ✓     M/M High MoS2 -200 to 315 Dry 0
MOLYKOTE D-10-GBL ✓     M/M Medium Graphite -40 to 340 Wet +
MOLYKOTE D-6024 ✓     M/M Medium MoS2 -40 to 310 Wet +
MOLYKOTE PA-744 ✓     M/M Medium MoS2 -75 to 300 Wet +
MOLYKOTE D-6818 ✓     M/M Medium MoS2 -60 to 240 Wet/Dry +
MOLYKOTE D-6927 ✓     M/M Medium PTFE -60 to 240 Wet/Dry +
MOLYKOTE D-6600 ✓     M/M, M/P, M/E Medium PTFE -40 to 260 Dry +
MOLYKOTE D-708 ✓     M/M, M/P, M/E Medium PTFE -180 to 240 Dry +
MOLYKOTE D-7708 ✓     M/M, M/P, M/E Medium PTFE -180 to 240 Dry +
MOLYKOTE D-96   ✓   P/P, P/M, P/E Low PTFE -40 to 150 Dry 0
MOLYKOTE D-96 UV   ✓   P/P, P/M, P/E Low PTFE -40 to 150 Dry 0
MOLYKOTE D-9630   ✓   P/P, P/M, P/E Low PTFE -40 to 120 Dry 0

1 M = metal; P = plastic; E = elastomer. The first letter in each pairing indicates the coated substrate.

2 Preferred working conditions. Oil/fuel resistance: + = good, 0 = limited, − = poor. Verify compatibility for the intended application.

Additional Dry-Film Lubricants and Coatings

The following products are also available in the Krayden Anti-Friction Coatings catalog. They include PTFE-based formulations, solid lubricants and protective coatings with different operating characteristics.

Product Technology / Type Typical Characteristics Service Temperature
MOLYKOTE D-321 Dry-film lubricant Air-curing coating for high-load metal sliding applications -180 to 450 °C
MOLYKOTE 557 Wax-like dry-film lubricant Clear, non-staining lubricating film with low friction See TDS
MOLYKOTE Z-POWDER MoS2 solid lubricant High-purity, free-flowing solid lubricant for dry lubrication -185 to 400 °C in air; up to 1100 °C in vacuum
BONDERITE L-GP 460 Graphite anti-seize lubricant Extreme-pressure lubrication for high-load applications Up to 538 °C
BONDERITE S-FN 309 PTFE dispersion Fast-drying low-friction coating for multiple substrates See TDS
BONDERITE S-FN 310A PTFE dry-film lubricant Low-friction release coating with enhanced wear life See TDS
BONDERITE S-FN 329 Resin-bonded PTFE Room-temperature curing for light-load moving components See TDS
BONDERITE S-FN 330 Dry-film lubricant Low-friction coating with corrosion resistance and stick-slip reduction Up to 150 °C
BONDERITE S-FN 333 Resin-bonded dry-film lubricant Bonded coating for low-friction applications See TDS
BONDERITE S-FN GP 1904 PTFE / Graphite Multi-substrate dry lubrication with corrosion and solvent resistance See TDS
BONDERITE S-OT 310B PTFE coating Low-friction lubrication with oil, solvent and chemical resistance See TDS

Protective and Wear-Resistant Coatings

These LOCTITE protective coatings are also included in the category. Their primary selection criteria relate to abrasion, corrosion, erosion and wear resistance rather than conventional dry-film lubrication.

Product Coating Type Primary Application Service Temperature
LOCTITE PC 7227 Brushable ceramic epoxy Wear and corrosion protection for pumps, tanks and industrial equipment Up to 100 °C dry / 90 °C wet
LOCTITE PC 7228 Low-friction protective coating Smooth, high-gloss surface protection See TDS
LOCTITE PC 7255 Two-part epoxy coating Industrial protective coating applications See TDS
LOCTITE PC 7303 High-temperature protective coating Protection of equipment operating at elevated temperatures -29 to 232 °C dry
LOCTITE PC 7317 Abrasion-resistant coating Protection from fine-particle abrasion and wear See TDS
LOCTITE PC 7319 Brushable / rollable coating Industrial equipment protection against wear -30 to 120 °C dry
LOCTITE PC 9313 Wear-resistant compound Build-up and protection of heavily worn surfaces See TDS

Technical guidance: Product selection should be confirmed against the manufacturer's technical data sheet and the actual substrate, load, speed, temperature and environmental conditions. Values shown are for general comparison and should not be used as manufacturing specifications.

Frequently asked questions

Frequently Asked Questions about Anti-Friction Coatings

How do anti-friction coatings differ from standard fluoropolymer paints?

Standard fluoropolymer paints prioritize corrosion resistance, chemical resistance, or decorative finish, offering limited load-bearing capacity. Engineering anti-friction coatings are formulated with specific ratios of sub-micron solid lubricants (MoS2, graphite, PTFE) and structural crosslinking resins (PAI, epoxy, silicates) designed to withstand high contact pressures, up to roughly 2,500 MPa, without flaking, delaminating, or wearing off prematurely.

Why is surface preparation critical before applying an AFC?

AFCs rely on combined mechanical and chemical bonding to the substrate. Adhesion depends directly on surface cleanliness and profile (Ra = 0.8 to 1.5 µm). Substrates must be degreased, grit-blasted (Al2O3), and ideally phosphated (for steel) or anodized (for aluminum) to maximize bond strength and prevent coating spallation under shear load.

Can an AFC be relubricated with standard wet oil or grease?

In most cases, yes. Cured AFCs are chemically stable and compatible with mineral and synthetic lubricants. Applying oil or grease to an AFC coating often provides secondary boundary protection if the wet fluid film breaks down. Solvents that degrade organic binders should still be avoided.

What is the optimal dry coating thickness for maximum wear life?

The ideal dry film thickness (DFT) for most load-bearing applications is between 10 µm and 20 µm. Coatings applied too thin (under 5 µm) yield reduced wear life and lower corrosion resistance, while coatings applied too thick (over 25 µm) are subject to cohesive shear failure, cracking, and potential tolerance issues in precision mechanisms.

Can a dry-film coating be applied over grease, oil, or another coating?

Normally not, unless the process specification explicitly allows it. Residual lubricant prevents adhesion. Existing paint, plating, phosphate, or anodize may be a designed underlayer, but its type, condition, and thickness must be approved. If repair or recoating is permitted, stripping, surface restoration, and maximum total thickness need to be defined.

How long does an anti-friction coating last?

Wear life is finite and application specific. It depends on the coating system, thickness, adhesion, contact pressure, sliding distance, oscillation amplitude, speed, temperature, atmosphere, contamination, counterface, and edge loading. ASTM D2625 and D2981 compare films under defined laboratory geometries, but changed conditions can change relative ranking, so cycle results should only be translated to service life through a validated correlation.


Learn more

Formulation

Before application and curing, an anti-friction coating consists of four functional components.

Solid Lubricant (10–30%)

MoS2 (high load/pressure), PTFE (low friction/light load), synthetic graphite (high temp/humidity stability), or h-BN (high dielectric strength/thermal stability).

Binder Matrix (10–30%)

Organic polymers (polyamide-imide, epoxy, phenolic, polyurethane) or inorganic compounds (silicates, phosphates) that anchor solid lubricants to the substrate.

Solvent Carrier (30–70%)

Organic solvents (NMP, MEK, xylene) or water (VOC-compliant systems) used to dissolve the binder and disperse solids for liquid spray, dip-spin, or brush application.

Additives (0–5%)

Specialized elements like corrosion inhibitors, dispersion agents, or catalysts added to enhance shelf life, curing speed, and environmental protection.

Anti-friction coating formulation

Common Binder Types

In an anti-friction coating (AFC), the binder is the resin matrix that locks solid lubricants, such as MoS2, graphite, or PTFE, to a substrate. Binders are divided into organic types (e.g., polyamide-imide, epoxy, phenolic) for toughness and chemical resistance, and inorganic types (e.g., silicate) for extreme high-heat performance.

Binder Class Curing Profile & Temp Max Operating Temp (°C) Load Capacity / Wear Life Chemical & Corrosion Resistance
Polyamide-Imide (PAI) Heat cure (200°C / 60 min) +260 Extreme (>2,000 MPa) Strong; solvent & acid resistant.
Epoxy Resin Heat cure (180°C / 30 min) +180 Very high Strong salt-spray corrosion protection.
Alkyd / Acrylic Air dry / ambient (20°C / 24 hrs) +100 Moderate Moderate; suitable for touch-up applications.
Inorganic Silicate Heat cure (300°C to 400°C) +450 to +650 High (brittle) Resistant to radiation & ultra-high vacuum.

Key Functions of the Binder

Adhesion

Bonds the dry-film lubricating pigments firmly onto metal, plastic, or elastomer surfaces.

Matrix Support

Holds solid lubricant particles in place under pressure and prevents them from flaking off.

Durability

Dictates the chemical, oil, and corrosion resistance of the final cured coating.


Advantages & Disadvantages

Advantages Disadvantages & Limitations
  • Completely dry, clean lubrication; minimal oil migration or dirt/dust buildup.
  • Stable performance in ultra-high vacuum (10⁻⁹ Torr) and radiation environments.
  • Provides long-term dry lubrication for un-relubricable or enclosed components.
  • Combines low friction performance with corrosion barrier protection.
  • Reduces oil/grease contamination of adjacent product or optics.
  • Thin films fit compact mechanisms.
  • Non-self-healing: once the physical dry film wears through, substrate wear accelerates.
  • Lower heat dissipation capability compared to circulating oil or grease systems.
  • Requires strict surface preparation (grit blasting, phosphating, precision baking).
  • Requires careful application tolerance control to maintain structural clearances.
  • Debris may be generated during run-in and wear.
  • Film thickness affects clearances, fits, and thread preload.

Anti-Friction Coating (AFC) Application Methodology

The performance, adhesion strength, and wear life of an AFC depend as much on the application process as on the coating's chemical formulation. Because AFCs function as thin structural tribological films, typically 10 µm to 20 µm dry film thickness, application requires a strict multi-stage workflow.

Anti-friction coating application methodology

1. Substrate Surface Preparation (Pre-Treatment)

1.1: Degreasing & Contaminant Removal

Objective: Remove all oils, rust preventatives, greases, and shop dirt.

Methods: Vapor degreasing (using chlorinated or fluorinated solvents), ultrasonic bath cleaning, or aqueous alkaline washing followed by a deionized water rinse and hot-air drying.

1.2: Mechanical Surface Roughing

Objective: Increase real surface area and establish a mechanical anchor profile for the resin binder.

Method: Fine grit-blasting using non-metallic, sharp-edged media such as aluminum oxide (Al2O3) or chilled iron grit (grit size: 120–220 mesh) at 0.2 to 0.4 MPa blast pressure.

1.3: Chemical Pre-Treatment (Conversion Coating)

Chemical conversion layers significantly enhance coating adhesion and provide secondary corrosion resistance underneath the solid lubricant film.

Substrate Material Chemical Conversion Process Layer Specification / Weight
Carbon Steel / Alloy Steel Manganese phosphating or zinc phosphating 3 to 10 g/m² (fine crystalline structure)
Stainless Steel Passivation or light sandblasting Citric / nitric acid, ASTM A967
Aluminum & Alloys Chromate conversion or hard anodizing MIL-DTL-5541 or Type III anodize (5–10 µm)
Titanium & Alloys Fluoride-phosphate conversion / alkaline etch AMS 2486 / AMS 2488

2. Coating Application Methods

2.1: Pneumatic Spray Application (HVLP)

Best For: Large components, complex geometries, low-to-medium production volumes, and high-precision applications requiring strict thickness control (e.g., engine pistons, aerospace valves).

Process Parameters: Atomization pressure 0.2 to 0.35 MPa; nozzle diameter 0.8 mm to 1.2 mm; spray distance 15 cm to 25 cm using cross-hatch strokes to prevent sags and pinholes.

Pneumatic spray application (HVLP)
Dip-spin coating process

2.2: Dip-Spin Coating (Centrifugal Bulk Processing)

Best For: High-volume processing of small components (screws, bolts, fasteners, clips, springs, brackets).

Process: Parts are submerged in an AFC fluid bath in a perforated basket, then spun at high speed so centrifugal force throws excess coating back into the bath, leaving a uniform, thin coating free of runs.

2.3: Dip-Drain / Immersion Coating

Best For: Long cylindrical parts, internal tube diameters, or symmetric rods where spraying can't access internal surfaces.

Process: The component is submerged in the AFC fluid and withdrawn at a controlled rate; withdrawal speed determines coating thickness via capillary force balance.

Dip-drain immersion coating
Selective screen and pad printing

2.4: Selective Screen / Pad Printing

Best For: Flat localized contact zones, gaskets, or bearing bushes where masking the rest of the component is cost-prohibitive.

Process: High-viscosity AFC formulations are forced through a patterned mesh screen or transferred via a silicone pad directly onto the friction face.


Flash-Off & Curing Mechanisms

After application, the wet coating layer must undergo a two-phase thermal transition: solvent evaporation followed by polymer crosslinking.

Flash-Off (Solvent Evaporation)

Before entering high-temperature cure ovens, coated parts must undergo a flash-off period at ambient or slightly elevated temperature (20°C to 80°C) for 10 to 15 minutes. This step allows volatile solvent carriers to evaporate gradually. Skipping flash-off causes trapped solvent to boil during curing, resulting in surface blisters, craters, and pinhole voids.

Curing (Binder Polymerization)

The curing cycle crosslinks the binder resin, permanently bonding the solid lubricant matrix to the pre-treated metal substrate.


Quality Control & Inspection Standards

To verify process stability and performance compliance, cured AFC coatings are subjected to three primary quality inspections.

Dry Film Thickness (DFT) Measurement

Standard: ISO 2178 / ASTM B499

Method: Magnetic-induction or eddy-current thickness gauges measure the dry film thickness.

Acceptance Criteria: Typical target range is 10 µm to 20 µm.

Dry film thickness measurement
Cross-hatch adhesion tape test

Cross-Hatch Adhesion Tape Test

Standard: ASTM D3359 Method B

Method: A lattice pattern of 6 or 11 cuts is made through the cured film to the substrate. Pressure-sensitive tape is applied firmly over the grid and pulled off abruptly at a 180° angle.

Acceptance Criteria: Rating 4B or 5B (zero to under 5% grid flaking at intersections).

Solvent Rub Test / Cure Verification

Standard: ASTM D5402

Method: A cloth soaked in methyl ethyl ketone (MEK) is rubbed back and forth across the cured coating surface for 50 double rubs under 10 N load.

Acceptance Criteria: No softening, dulling, or transfer of coating material to the cloth.

Solvent rub cure verification test

Key Sector Applications & Engineering Functions

1. Automotive & Powertrain Engineering

Engine Piston Skirts: Heat-cured MoS2 bound in polyamide-imide (PAI) resin reduces cold-start hydrodynamic drag and helps protect against cylinder wall scuffing.

Door Latches, Hinges & Window Regulators: PTFE/epoxy coatings deliver maintenance-free, long-term dry sliding for over 100,000 cycles without transferring oil or attracting dust.

Brake Clips & Anti-Squeal Plates: Thermally stable PTFE/epoxy coatings help prevent stick-slip friction and pad drag without trapping abrasive brake dust.

Piston skirt coating, door latches, hinges, window regulators, caliper springs and brake clips

2. Aerospace, Defense & Space Systems

Spacecraft solar array gimbals, deployment hinges, jet engine lock-nuts and fasteners

Spacecraft Solar Array Gimbals & Deployment Hinges: Inorganic silicate-bound MoS2 coatings operate reliably in ultra-high vacuum (10⁻⁹ Torr) and radiation environments with minimal outgassing.

Jet Engine Lock-Nuts & Fasteners: High-purity MoS2 in a PAI binder helps eliminate thread galling under severe thermal cycling (-55°C to +450°C) and supports predictable breakout torque.

3. Oil & Gas, Marine & Subsea Equipment

Subsea Gate Valves & Actuator Stems: Fluoropolymer (PTFE) and MoS2 blended with epoxy binders withstand extreme contact pressures (up to roughly 2,500 MPa) while providing extended ASTM B117 salt spray corrosion barrier protection.

Tubular Threaded Connections (OCTG): Dry-film coatings replace traditional heavy metal pipe dope, helping prevent thread galling during high-torque makeup.

Tubular threaded connections (OCTG)

4. Semiconductor Manufacturing & Vacuum Systems

Cleanroom linear guide

Cleanroom Wafer Transfer Arms & Linear Guides: PAI-bound PTFE dry films provide particle-free sliding motion in Class 1/10 cleanrooms, helping eliminate oil aerosol contamination on silicon wafers.

5. Industrial Machinery, Textiles & Consumer Goods

Textile Yarn Feeders & Printing Equipment: PTFE dry coatings help prevent paper fibers, lint, and dust from adhering to sliding guides, reducing equipment jams.

Solenoid Plungers & Pneumatic Valves: Ultrathin (5 µm to 10 µm) air-drying acrylic/PTFE coatings reduce electrical switching hysteresis and help eliminate stiction.

Textile yarn feeders, printing equipment, solenoid plungers and pneumatic valves

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers